Max. Limited Temperatur |
Material Required for Estimating |
CA | PLC | CCS | M.O.R | Installations | Main Applications | ||||||||||||||||
¢ªC | kg/m3 | Al203 (%) |
SiO2 (%) |
Ca0 (%) |
SiC (%) |
110¢ªC (%) |
1,000¢ªC (%) |
1,350¢ªC (%) |
1,400¢ªC (%) |
1,500¢ªC (%) |
110¢ªC (%) |
1,000¢ªC (%) |
1,350¢ªC (%) |
1,400¢ªC (%) |
1,500¢ªC (%) |
110¢ªC (%) |
1,000¢ªC (%) |
1,350¢ªC (%) |
1,400¢ªC (%) |
1,500¢ªC (%) |
|||
HSC-18SC | 1,800 | 3,250 | 93 | 3 | 2 | -0.03 | -0.43 | 1,300 | 1,400 | 220 | 300 | ||||||||||||
HSC-18RA | 1,800 | 3,200 | 90 | 2 | 5 | -0.06 | -0.3 | 1,000 | 1,100 | 200 | 250 |
Max. Limited Temperatur |
Material Required for Estimating |
CA | PLC | CCS | M.O.R | Installations | Main Applications | ||||||||||||||||
¢ªC | kg/m3 | Al203 (%) |
SiO2 (%) |
Ca0 (%) |
SiC (%) |
110¢ªC (%) |
1,000¢ªC (%) |
1,350¢ªC (%) |
1,400¢ªC (%) |
1,500¢ªC (%) |
110¢ªC (%) |
1,000¢ªC (%) |
1,350¢ªC (%) |
1,400¢ªC (%) |
1,500¢ªC (%) |
110¢ªC (%) |
1,000¢ªC (%) |
1,350¢ªC (%) |
1,400¢ªC (%) |
1,500¢ªC (%) |
|||
HSC-18 | 1,800 | 3,200 | 90 | - | 2 | -0.06 | 800 | 900 | 200 | 240 | 350 | Cement Kiln, Hot blast furnace, COKE Oven, etc Various furnac |
|||||||||||
HSC-17 | 1,700 | 2,750 | 75 | 20 | 2 | -0.05 | 650 | 680 | 110 | 120 | 130 | ||||||||||||
HSC-85AL | 1,700 | 2,900 | 85 | 8 | - | -0.03 | 53 | 680 | 120 | ||||||||||||||
HSC-16H-W2 | 1,600 | 2,560 | 57 | 38 | 2 | 0.00 | -0.15 | 900 | 950 | 100 | 200 | ||||||||||||
HSC-16S-W2 | 1,600 | 2,640 | 65 | 30 | 1 | -0.02 | -0.03 | 920 | 110 | 180 | 180 | ||||||||||||
HSC-16SF-W2 | 1,600 | 2,360 | 40 | 55 | 2 | -0.03 | -0.09 | 770 | 900 | 200 | 130 | ||||||||||||
HSC-16H-W2 | 1,600 | 2,700 | 57 | 38 | 2 | -0.03 | 0.50 | 800 | 920 | 150 | 250 | 270 | |||||||||||
HSC-16 | 1,600 | 2,600 | 55 | 40 | 2 | -0.04 | 0.50 | 610 | 630 | 180 | 110 | 120 | |||||||||||
HSC-15 | 1,500 | 2,400 | 50 | 45 | 2 | -0.05 | -0.05 | 450 | 450 | 100 | 100 | ||||||||||||
HSC-FBW | 1,600 | 2,500 | 56 | 38 | 2 | -0.03 | -0.05 | 1,000 | 1,500 | 100 | 250 | 100 | |||||||||||
HSC-15G | 1,500 | 2,200 | 50 | 45 | 4 | -0.10 | -0.20 | 400 | 350 | 230 | 250 | Spray | |||||||||||
USC-DC10 | 1,500 | 91 | 2 | 50 | 60 | Finex Reactor |
Max. Limited Temperatur |
Material Required for Estimating |
CA | PLC | CCS | M.O.R | Installations | Main Applications | ||||||||||||||||
¢ªC | kg/m3 | Al203 (%) |
SiO2 (%) |
Ca0 (%) |
SiC (%) |
110¢ªC (%) |
1,000¢ªC (%) |
1,350¢ªC (%) |
1,400¢ªC (%) |
1,500¢ªC (%) |
110¢ªC (%) |
1,000¢ªC (%) |
1,350¢ªC (%) |
1,400¢ªC (%) |
1,500¢ªC (%) |
110¢ªC (%) |
1,000¢ªC (%) |
1,350¢ªC (%) |
1,400¢ªC (%) |
1,500¢ªC (%) |
|||
MMCT-95 | 1,800 | 3,100 | 95 | 0.00 | 0.06 | 0.4 | 400 | 750 | 800 | 75 | 150 | 150 | Casting, Vibrating | Ladle, RH-OB Snorkel, Others |
|||||||||
MMCT-85 | 1,700 | 2,800 | 85 | 3 | -0.03 | -0.10 | 0.4 | 400 | 700 | 800 | 75 | 100 | 150 | Casting, Vibrating | |||||||||
MMCT-75 | 1,600 | 2,500 | 75 | 10 | -0.06 | -0.15 | 0.3 | 350 | 600 | 900 | 70 | 100 | 200 | Casting, Vibrating |
Max. Limited Temperatur |
Material Required for Estimating |
CA | PLC | CCS | M.O.R | Installations | Main Applications | ||||||||||||||||
¢ªC | kg/m3 | Al203 (%) |
SiO2 (%) |
Ca0 (%) |
SiC (%) |
110¢ªC (%) |
1,000¢ªC (%) |
1,350¢ªC (%) |
1,400¢ªC (%) |
1,500¢ªC (%) |
110¢ªC (%) |
1,000¢ªC (%) |
1,350¢ªC (%) |
1,400¢ªC (%) |
1,500¢ªC (%) |
110¢ªC (%) |
1,000¢ªC (%) |
1,350¢ªC (%) |
1,400¢ªC (%) |
1,500¢ªC (%) |
|||
SFC-90SC | 1,800 | 3,100 | 95 | 4 | -0.03 | -0.10 | -0.35 | 950 | 1,000 | 1,100 | 170 | 230 | 240 | Self Leveling | Cement Klin, etc. | ||||||||
SFC-90W | 1,800 | 3,200 | 95 | 4 | -0.03 | -0.10 | -0.35 | 1,000 | 1,100 | 1,150 | 180 | 240 | 250 | Self Leveling | |||||||||
SFC-90SC | 1,800 | 3,050 | 87 | 5 | 5 | -0.03 | -0.06 | -0.09 | 800 | 900 | 1,000 | 150 | 220 | 230 | Self Leveling | ||||||||
SFC-UL90S | 1,800 | 3,200 | 87 | 6 | 5 | -0.03 | -0.30 | -0.15 | 650 | 950 | 1,100 | 100 | 250 | 280 | Self Leveling | ||||||||
SFC-70R | 1,700 | 2,480 | 75 | 17 | -0.03 | -0.06 | 52 | 420 | 760 | 100 | 70 | 150 | Self Leveling | ||||||||||
SFC-165 | 1,650 | 2,450 | 61 | 34 | -0.03 | 0.12 | 550 | 800 | 850 | 110 | 120 | 130 | Self Leveling | ||||||||||
SFC-85 | 1,800 | 2,800 | 85 | 4 | 3 | -0.03 | 0.60 | 750 | -1300 | 120 | 230 | Self Leveling | |||||||||||
SFC-70R | 2,610 | 18 | 73 | -0.03 | -0.09 | 530 | 900 | 1,200 | 100 | 200 | 250 | Self Leveling | |||||||||||
SFC-60 | 2,570 | 22 | 63 | -0.03 | -0.09 | 500 | 850 | 1,100 | 90 | 180 | 230 | Self Leveling | |||||||||||
Max. Limited Temperatur |
Material Required for Estimating |
CA | PLC | CCS | M.O.R | TC | Installations | Main Applications | ||||||||||||||||||
¢ªC | kg/m3 | Al203 (%) |
SiO2 (%) |
110¢ªC (%) |
1,000¢ªC (%) |
1,350¢ªC (%) |
1,500¢ªC (%) |
110¢ªC (kg/cm) |
500¢ªC (%) |
1,000¢ªC (kg/cm) |
1,350¢ªC (kg/cm) |
1,500¢ªC (kg/cm) |
110¢ªC (kg/cm) |
500¢ªC (%) |
1,000¢ªC (kg/cm) |
1,350¢ªC (kg/cm) |
1,400¢ªC (kg/cm) |
1,500¢ªC (kg/cm) |
200¢ªC (kcal/m.h.¢ªC) |
540¢ªC (kcal/m.h.¢ªC) |
800¢ªC (kcal/m.h.¢ªC) |
|||||
INCT-170 | 1,700 | 1,750 | 92 | -0.03 | -0.50 | -0.50 | 150 | 210 | 70 | 80 | Casting, Troweling |
Deoxidizing gas resistance High temp |
||||||||||||||
INCT-160 | 1,600 | 1,600 | 63 | 28 | -0.03 | 150 | 240 | 45 | 90 | 0.52 | 0.57 | 0.62 | Casting, Troweling |
High temperature | ||||||||||||
INCT-140 | 1,400 | 1,350 | 50 | 36 | -0.06 | -0.25 | 55 | 40 | 40 | 30 | 30 | 0.34 | 0.38 | 0.42 | Casting, Troweling |
Fireproof insulating | ||||||||||
ICT-135S | 1,350 | 900 | 43 | 38 | -0.06 | -0.25 | 60 | 75 | 15 | 15 | 0.25 | 0.28 | 0.31 | Casting, Troweling |
High temperature Low thermalconductivity |
|||||||||||
INCT-135N | 1,350 | 1,400 | 38 | 48 | -0.06 | -0.45 | 60 | 20 | 30 | 15 | 0.34 | 0.38 | 0.42 | Casting, Troweling |
High temperature Low thermalconductivity |
|||||||||||
INCT-120S | 1,200 | 900 | 33 | 43 | -0.06 | -0.35 | 40 | 40 | 20 | 15 | 0.2 | 0.24 | 0.28 | Casting, Troweling |
High temperature Low thermalconductivity |
|||||||||||
INCT-120N | 1,200 | 1,200 | 25 | 53 | -0.06 | -0.20 | 50 | 35 | 20 | 10 | 0.32 | 0.36 | 0.4 | Casting, Troweling |
High temperature Low thermalconductivity |
|||||||||||
INCT-110S | 1,100 | 800 | 30 | 37 | -0.06 | -0.80 | 40 | 25 | 10 | 20 | 0.14 | 0.17 | 0.21 | Casting, Troweling |
general furnaces | |||||||||||
INCT-110N | 1,100 | 1,150 | 25 | 55 | -0.06 | -0.43 | 50 | 40 | 12 | 15 | 0.29 | 0.31 | 0.35 | Casting, Troweling |
Low temperature Various furnaces |
|||||||||||
INCT-100S | 1,000 | 700 | 30 | 35 | -0.06 | 15 | 5 | 8 | 3 | 3 | 0.13 | 0.15 | 0.21 | Casting, Troweling |
Low temperature Various furnaces |
|||||||||||
INCT-100N | 1,000 | 1,250 | 25 | 50 | -0.06 | -0.60 | 70 | 45 | 20 | 5 | 10 | 0.25 | 0.28 | 0.31 | Casting, Troweling |
Low temperature Various furnaces |
||||||||||
INCT-80S | 800 | 450 | 28 | 38 | -0.06 | -0.60 | 6 | 6 | 3 | 6 | 3 | 0.12 | 0.19 | Casting, Troweling |
Low temperature Various furnaces |
|||||||||||
Max. Limited Temperatur |
Material Required for Estimating |
CA | PLC | CCS | M.O.R | TC | Installations | Main Applications | ||||||||||||||||||
¢ªC | kg/m3 | Al203 (%) |
SiO2 (%) |
110¢ªC (%) |
1,000¢ªC (%) |
1,350¢ªC (%) |
1,500¢ªC (%) |
110¢ªC (kg/cm) |
500¢ªC (%) |
1,000¢ªC (kg/cm) |
1,350¢ªC (kg/cm) |
1,500¢ªC (kg/cm) |
110¢ªC (kg/cm) |
500¢ªC (%) |
1,000¢ªC (kg/cm) |
1,350¢ªC (kg/cm) |
1,400¢ªC (kg/cm) |
1,500¢ªC (kg/cm) |
200¢ªC (kcal/m.h.¢ªC) |
540¢ªC (kcal/m.h.¢ªC) |
800¢ªC (kcal/m.h.¢ªC) |
|||||
GUN-140L | 1,400 | 1,500 | 47 | 32 | -0.15 | -0.40 | 55 | 25 | 20 | 12 | 0.4 | 0.42 | 0.48 | Gunning | Fireproof Insulating Part |
|||||||||||
GUN-1356 | 1,350 | 1,450 | 37 | 41 | -0.10 | -0.50 | 35 | 20 | 15 | 10 | 0.4 | 0.42 | 0.48 | Gunning | Fireproof Insulating Part |
|||||||||||
GUN-120L | 1,200 | 1,300 | 34 | 47 | -0.10 | -0.60 | 35 | 30 | 15 | 10 | 0.3 | 0.32 | 0.34 | Gunning | General Uses | |||||||||||
GUN-110L | 1,100 | 1,100 | 29 | 39 | -0.10 | -0.90 | 30 | 20 | 15 | 9 | 0.24 | 0.26 | 0.28 | Gunning | General Uses | |||||||||||
GUN-100L | 1,000 | 1,000 | -0.20 | 10 | 8 | 0.2 | 0.23 | 0.24 | Gunning | Low Temperature | ||||||||||||||||
MIX-1(1:4) | 1,100 | 1,500 | 0.00 | -0.8 | 100 | 55 | 30 | 20 | 0.3 | 0.45 | Gunning,Casting(UOP) | Petrochemical plant Heater, boiler |
||||||||||||||
MIX-2(1:2:4LHV) | 1,000 | 800 | -0.20 | -1.2 | 20 | 10 | 10 | 5 | 0.18 | 0.23 | Gunning,Casting(UOP) | Petrochemical plant Heater, boiler |
||||||||||||||
MIX-3(1:6) | 1,000 | 550 | -0.25 | -0.25 | 10 | 6 | 5 | 3 | 0.13 | 0.14 | Gunning,Casting(UOP) | Petrochemical plant Heater, boiler |
||||||||||||||
Max. Limited Temperatur |
Material Required for Estimating |
CA | PLC | CCS | M.O.R | Water Required for Casting |
Installations | Main Applications | |||||||||||
¢ªC | kg/m3 | Al203 (%) |
SiO2 (%) |
110¢ªC (%) |
500¢ªC (%) |
1,000¢ªC (%) |
110¢ªC (kg/cm2) |
500¢ªC (kg/cm2) |
1,000¢ªC (kg/cm2) |
110¢ªC (kg/cm2) |
1,000¢ªC (kg/cm2) |
1,350¢ªC (kg/cm2) |
% | ||||||
APC-120 | 1,200 | 2,000 | 40 | 55 | -0.10 | -0.25 | -0.50 | 120 | 300 | 350 | 50 | 80 | 100 | WaterGlass | 15 | Casting, Vibrating | Chemical Plant | ||
APC-80 | 800 | 1,900 | 30 | 65 | -0.10 | -0.30 | 120 | 250 | 45 | 60 | WaterGlass | 15 | Casting, Vibrating | Chemical Plant | |||||
APC-50 | 500 | 1,850 | 25 | 70 | -0.20 | 140 | 200 | 300 | 75 | 90 | WaterGlass | 18 | Casting, Vibrating | Chemical Plant | |||||
APC-120G | 1,200 | 2,200 | 42 | 53 | -0.10 | -0.40 | -0.60 | 80 | 250 | 30 | 70 | 100 | Spray | Chemical Plant | |||||
APC-100G | 1,000 | 2,200 | 18 | 69 | -0.20 | -0.30 | 250 | 280 | 70 | 80 | Spray | Chemical Plant | |||||||
APC-80G | 800 | 2,100 | 27 | 68 | -0.10 | -0.50 | 70 | 20 | 25 | 55 | Spray | Chemical Plant | |||||||
APC-50G | 500 | 250 | 31 | 62 | -0.20 | 120 | 180 | 70 | 80 | Spray | Chemical Plant | ||||||||