Brand | Refractoriness | CA | Bonding Stength | Grain Size | Setting Time | Main Applications | ||||||||||
SK | Al203 (%) |
Si0 (%) |
SiC (%) |
SiC+C (%) |
Zr0 (%) |
Fe0 (%) |
110¢ªC (kg/cm2) |
1,000¢ªC (kg/cm2) |
1,400¢ªC (kg/cm2) |
1,500¢ªC (kg/cm2) |
+0.5mm (%) |
+0.3mm (%) |
-0.07mm (%) |
min | ||
IMO-1 | 31 | 10 | 40 | LBK23,LBK28, Blast Fumace stove |
||||||||||||
ZM-1 | 35 | 55≤ | 20 | 15 | 40 | 20≥ | 50≤ | Zircon ladle brick | ||||||||
APM-1 | 60≤ | 20 | 10 | For Acid-proof bricks | ||||||||||||
SP-85W | 39 | 85≤ | 2≥ | 50 | 60 | 70 | 2≥ | 50≤ | General brick incinerator brick | |||||||
SP-3000 | 34 | 45≤ | 2≥ | 90 | 80 | 2≥ | 50≤ | Brick | ||||||||
ASM-40 | 40 | 95 | 3≥ | 20 | 40 | 10≥ | 50≤ | SK-40 Brick | ||||||||
ASM-39 | 39 | 85 | 3≥ | 20 | 40 | 10≥ | 50≤ | SK-39 Brick | ||||||||
ASM-38 | 38 | 75 | 3≥ | 20 | 40 | 10≥ | 50≤ | SK-38 Brick | ||||||||
ASM-37 | 37 | 65 | 3≥ | 20 | 40 | 10≥ | 50≤ | SK-37 Brick | ||||||||
ASM-36 | 36 | 55 | 3≥ | 20 | 40 | 10≥ | 50≤ | SK-36 Brick | ||||||||
ASM-35 | 35 | 50 | 3≥ | 20 | 40 | 10≥ | 50≤ | SK-35 Brick | ||||||||
ASM-34 | 34 | 45 | 3≥ | 10 | 30 | 10≥ | 50≤ | SK-34 Brick | ||||||||
BM-1 | 5 | 15 | 30≤ | A1-A4, B1-B4, Brick | ||||||||||||
BM-2 | 5 | 7 | 15 | 30≤ | A5, B5, C5, LW20, LW23 | |||||||||||
BM-3 | 5 | 7 | 10 | 30≤ | A6, A7, B6, B7, C2, D3, LW24 | |||||||||||